- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Setup or cover-up?
Too much bending pressure can but shouldnt compensate for poor tooling setup
- By William Q. Tingley III
- March 11, 2008
- Article
- Tube and Pipe Fabrication
Even though we are in the age of CNC machinery, the old phrase "the tools make the bend" is as relevant today as ever. As tube bending applications have become more extreme, tooling design, setup, and maintenance have returned to a position of central importance. In rotary draw bending, four simple setup steps, executed precisely and in the correct order, will help you maximize bend quality, tool life, and process control.
Many tube bending machine operators rely on machine features more than they should. Modern features on tube benders, especially pressure die assist, permit many operators to obtain adequate results without mastering tooling setup. Many controls on CNC bending machines were devised to make difficult applications practical. Many operators use these controls to overcome the limitations of poor setup practices on routine applications.
This over-reliance on the machine's controls "squeezes" the tube into the desired shape through use of excessive radial force at the point of bend. Because this approach works against the axial tension on the tube that is natural to the rotary draw process, it requires high machine pressure to force the part into shape. This results in a tradeoff: High pressure at the point of bend decreases tool life, process control, or both.
It is not necessary to sacrifice tool life or process control for better bend quality. You can maximize all three of these objectives with a little time and effort. It's a matter of using a four-step procedure that precisely positions the tooling:
- Move the mandrel forward.
- Lower the pressure die setting.
- Rake the wiper tip.
- Adjust the pressure die assist setting as needed.
The Four-step Setup
The trick to implementing the four-step setup successfully is understanding that each step addresses just one aspect of bend quality.
Accurate mandrel nose placement ensures a stable round cross section throughout the arc of the bend. A correct direct (or radial) pressure setting of the pressure die prevents buckling on the inside radius. A wiper tip properly raked away from the line of tangency prevents the wrinkle or series of small wrinkles that can form at the terminal end of the inside radius. And, finally, a balanced pressure die assist setting will push out the outside radius sufficiently to mitigate flattening and to eliminate any terminal hump.
Not all draw bending applications require a mandrel, a wiper, or the pressure die assist feature. However, understanding each of them can help you troubleshoot problems more accurately and quickly and determine the need for one of these if it is absent. Furthermore, applying these steps in the right sequence helps overcome a common troubleshooting hurdle: One tool improperly set up can mask another.
Step 1: Move the Mandrel Forward
The mandrel is the central tool in the draw bending setup. It is your primary means of controlling the flow of tubing material at the point of bend. To understand the best placement of the mandrel nose, it is necessary to understand the difference between the line of tangency and the point of bend.
The line of tangency is a theoretical plane fixed in space (see Figure 1). It is perpendicular to the plane of bend and divides the bend arc from the tangent. On the other hand, the point of bend is an indefinite region surrounding the line of tangency in which the tubing material is in a plastic state.
As the clamps draw the tube around the bend die, the tube wall thickens along the inside radius (intrados) and thins along the outside radius (extrados). The purpose of the mandrel nose is to cover this region of flowing material and ensure a consistently round cross section by mitigating the simultaneous compressing and stretching of the tube wall.
Because the point of bend extends past the line of tangency, so too must the mandrel nose to support it (seeFigure 2). If it does not, it will not provide the necessary control over the tube wall.
The result is buckling and excessive flattening.
While more direct pressure from the pressure die often can prevent buckling along the inside radius, this makes another problem worse: It increases the drag on the outside radius, exacerbating the flattening of the outside radius. Therefore, placing the mandrel nose past the line of tangency is critical, because proper placement eliminates buckling and minimizes flattening.
Several factors come into play in calculating proper mandrel placement:
- Tube outside diameter (OD)
- Wall thickness (WT)
- Centerline bending radius (r)
- Mandrel nose diameter (Md)
- Mandrel nose radius (Mr)
Consider a tube that is 2 in. OD by 0.049 in. thick, to be bent to a 4-in. centerline bending radius.
- Find the mandrel nose diameter: Md= OD - (WT x 2.21) = 2 - (0.049 x 2.21) = 1.8917.
- Find the mandrel nose radius. First, find the wall factor: Fw= OD/WT = 2 / 0.049 = 41.
- If Fw < 50, Mr = Md x 0.1
- If Fw >50, Mr = Md x 0.02
In this example, Fw < 50, so Mr = 1.8917 x 0.01 = 0.18917.
Using the Pythagorean theorem is the key to calculating the maximum depth for the mandrel. The theorem states that for any right triangle, the sum of the squares of the two short sides equals the square of the hypotenuse:
a2 + b2= c2
Because we want to find b, we can rearrange the equation:
b2 = (c2 - a2)
Variable c is the linear distance from the center of the bend die to the inside of the far tube wall (in other words, the sum of the centerline bending radius plus half of the tube's OD minus the wall thickness), so it is rendered as r + (OD/2) - WT (see Figure 3). Variable a is the linear distance from the center of the bend die to the far edge of the mandrel body (in other words, the sum of the centerline bending radius plus half of the mandrel's diameter), so it is rendered as r + (Md/2).
The formula for finding the proper mandrel setting is a variation on the Pythagorean theorem. After finding the difference between the squares of the two linear distances, add the radius of the mandrel nose, Mr.
b = SQRT{ [r + (OD/2) - WT]2 – [ r + (Md/2)]2} + Mr
b = SQRT { [4 + (2/2) – 0.049]2 – [4 + 1.8917/2]2} + 0.18917
b = SQRT { [4.9510]2 – [4.9459]2} + 0.18917
b = 0.4148
So for this example, the maximum mandrel depth is approximately 0.42 in. (3/8 in.) past the line of tangency. Placing the mandrel somewhere between one-half and two-thirds of the maximum usually is best. The less rigid the material, the deeper the placement must be.
How far forward is too far forward for mandrel placement? At some point the outside line of the mandrel nose will intersect the outside radius of the bend and force the tubing material to form over the contour of the nose and perhaps the mandrel balls. This point is fairly deep into the bend.
This is the mandrel forward principle of this setup procedure. This step should produce a bend that has a consistent cross section throughout most of the arc. The most serious problem you might have is buckling throughout the inside radius. If your mandrel nose is stable at the proper depth and its diameter is the right size for the application, then go to the next step to determine the correct direct pressure die setting.
Step 2: Lower the Pressure Die Setting
Because a properly set mandrel does most of the work in controlling the shape of the tube during the bending process, the pressure die's job is merely to keep the tube in place—that is, it should apply just enough pressure to prevent the tube from pulling away from the bend die during the bend. (If it does pull away, then the inside radius will buckle into the gap created.)
Whether it is mechanical or hydraulic, the pressure die applies a radial force against the tube at the point of bend. Because this radial force is perpendicular to the natural axial flow of material in the draw bending process, drag results.
Too much drag results in terminal humps and excessive flattening of the outside radius. Too much drag is usually the culprit when the tube slips from the clamp dies. Thus, the objective is to eliminate as much drag as possible by determining the lowest amount of direct (radial) pressure needed to prevent buckling.
Most round tube applications up to 3 in. in diameter, whether mild steel, stainless steel, aluminum, or copper, require just 400 to 1,200 pounds per square inch (PSI) of direct pressure to accomplish this. Square and rectangular tubes (especially if bent the hard way) require higher pressures, and so do copper-nickel, superalloy, and some stainless steels.
No simple formula exists for calculating the optimum setting for every shape and material, but a little experimentation will yield substantial benefits.
For a typical 3-in.-capacity machine, use the following guidelines:
- 400-500 PSI for soft materials (soft aluminum, soft copper, and hydroformable low-carbon steel)
- 600-700 PSI for midrange materials (high-carbon steels, hard aluminum, and hard copper)
- 900-1,000 PSI for the hardest materials (titanium, nickel, stainless steel, superalloys such as INCONEL®, and nonround tubing of any material)
If continuous wrinkling or a buckle forms on the inside radius, increase the direct pressure setting in increments of 50 to 100 PSI until the problem disappears. If the inside radius has no noticeable deformation, consider dropping the direct pressure. After you determine the minimum direct pressure for the application, you can use it as a suitable reference point for future setups of the same application and a guideline for other applications.
This concludes forward mandrel and low pressure concepts. Remaining imperfections, such as a terminal inside radius wrinkle or terminal outside radius hump, likely will be remedied by the last two steps of the setup procedure.
Step 3: Rake the Wiper Tip
The wiper's job is to prevent a wrinkle from forming at the end of the bend. If no wrinkle appears at the terminal end of an otherwise smooth inside radius, a wiper is unnecessary. Skip this step and proceed to Step 4.
The wiper fills the gap behind the line of tangency between the inside edge of the tube and the curve of the bend die cavity. If the tube wall is not sufficiently rigid, it will bulge outward to fill this gap. With enough pressure on the direct pressure die, this bulge will flatten out between the bend die cavity and the mandrel nose as the tube is drawn through the line of tangency. But, at the end of the bend, if the bulge is not drawn through and flattened, it can form a wrinkle or a small series of wrinkles. Properly set, the tip of the wiper will catch the top of this terminal bulge before it sets into a wrinkle.
First, find the natural resting position of the wiper at zero rake; then determine the maximum rake for that application. To do this, hold a straightedge at the bottom of the grip section of the bend die cavity. With the wiper loosely mounted on the wiper post, bring in the wiper so that the bottom of its cavity also lines up with the straightedge. The wiper is now at zero rake. To find its natural resting position, gently slide the wiper along the straightedge toward the line of tangency until you meet some resistance. Determine if the feathered edge of the wiper tip is in complete contact with the bend die cavity. If so, you have found the natural fit. If not, apply slightly more force until the feathered edge is securely backed by the bend die cavity.
If you must use considerable force to find a fit, most likely the wiper is improperly cut or you are trying to get the tip too close to the line of tangency. The latter is a common problem because it looks better when the wiper is at the line of tangency; however, most wipers are not cut to permit such a setting, nor is it necessary if the purpose of the wiper is limited to containing the terminal bulge.
Once you have found the natural zero rake position, rake the wiper by rotating the tip along the bend die cavity away from the line of tangency. You can increase rake in this manner so long as the terminal bulge does not set into a wrinkle. Once you have set the rake, you can measure the linear distance along the bend die cavity from the wiper tip to the line of tangency. Provided that replacement wiper tips are of the same design and manufacture, you can short-cut this step in the setup by setting a new wiper at this distance.
Note that raking the wiper applies only to low-pressure bending applications. Also, if the wiper is raked, the feathered edge should be cut to "simple-sweep" geometry. This is the most common geometric form. High-pressure jobs require zero rake and a feathered edge with offset geometry, not simple-sweep geometry.
Step 4: Adjust the Pressure Die Assist setting
Like the wiper, pressure die assist is not always necessary. Its job is to prevent terminal humps and excessive flattening along the outside radius. If the outside radius is acceptable, you do not need pressure die assist. Turn it off or set it to a neutral pressure, depending on your machine. Otherwise, start from neutral pressure and increase the assist until the flaws disappear.
Keep in mind that many CNC tube bending machines have both assist pressure and boost pressure. The term boost generally means a type of axial pressure applied during the bend to the entire circumference of the tube by means of clamps behind the pressure die. Using this type of pressure forces material through the line of tangency to feed both the intrados and the extrados. Assist, on the other hand, feeds material only into the extrados, which is useful in decreasing flattening and wall thinning.
Troubleshooting
A big advantage of the four-step setup procedure is that it facilitates troubleshooting. Most defects in a tube bend can be traced to the setup, and most setup defects correlate with a problem in one of the four steps. Therefore, after you have identified the nature of the defect, you will have a specific setup parameter you should examine first.
About the Author
William Q. Tingley III
1009 Ottawa Ave. N.W.
Grand Rapids, MI 49503
800-284-8823
About the Publication
Related Companies
subscribe now
The Tube and Pipe Journal became the first magazine dedicated to serving the metal tube and pipe industry in 1990. Today, it remains the only North American publication devoted to this industry, and it has become the most trusted source of information for tube and pipe professionals.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 05/14/2024
- Running Time:
- 62:12
Cameron Adams of Laser Precision, a contract metal fabricator in the Chicago area, joins the podcast to talk...
- Trending Articles
Making the move from hard automation to robotic welding
Zekelman Industries to invest $120 million in Arkansas expansion
Brushless copper tubing cutter adjusts to ODs up to 2-1/8 in.
HGG Profiling Equipment names area sales manager
Students learn fabrication one piece at a time
- Industry Events
Laser Welding Certificate Course
- May 7 - August 6, 2024
- Farmington Hills, IL
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,