- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Pressure matters in abrasive waterjet cutting
How pressure affects cutting speed, kerf width, and abrasive use
- By Pradeep Nambiath, Ph.D.
- November 29, 2016
- Article
- Waterjet Cutting
Over the past three decades, abrasive waterjet machines have evolved from a relatively crude cutting tool in the 1980s to a refined machine tool used in sectors ranging from aerospace to the food industry.
This evolution has occurred in major part because of material development, efficient system designs, better control of the waterjet tool, and the natural progression to higher pressure.
How Pumps Work
During the initial two decades of waterjet cutting,
relatively small increments in pump pressures up to 60,000 PSI (4,100 bar) were typical; during the last decade, pump pressures jumped to pressures of 90,000 PSI (6,200 bar).
Modern abrasive waterjet machines use either an intensifier pump or direct- drive pump to generate the high pressures required to create a high-velocity cutting stream. Intensifier pumps (see Figure 1) use hydraulics and what’s known as the intensification principle, as shown in Figure 2. This principle is similar to what is observed in a hydraulic press, where pressure times area, or P × A, is a constant.
Oil pumped into the hydraulic cylinder at low pressures pushes against the piston, which has a plunger connected to it. The area of the piston is 20 to 30 times the area of the end of the plunger. So the lower pressure over the larger area of the piston is converted to a higher pressure over the smaller area of the plunger. This generates water pressures ranging from 60 KSI to 90 KSI exiting from the check valve end of the cylinder.
Intensifier pumps are also referred to as constant-pressure pumps because of their ability to maintain the commanded pressure independent of the state the pump is in, be it stroking or idle. The idle condition is usually a result of the valve closing the flow as the head traverses between cuts or reaches the end of a cut.
Direct-drive pumps use a crankshaft to move plungers that pressurize water up to 60 KSI, very similar to how pressure washers operate. Direct-drive pumps, also referred to as constant-flow pumps, require careful control during idling to prevent overpressurizing the system.
How Abrasive Waterjets Work
Abrasive waterjet cutting works on the principle of using high-pressure water generated by the pump to create a high-velocity stream through a jewel orifice. The jewel is the point where high-pressure water transitions to high-velocity water. This waterjet creates a vacuum in a mixing chamber where abrasive particles are entrained into the high-velocity stream. Through momentum transfer, abrasive particles accelerate to speeds close to that of the water stream and are refocused into a cohesive cutting stream through a focusing tube adjacent to the mixing chamber (see Figure 3).
This mix of water and abrasive exiting the mixing tube is the visible cutting jet. In metals, the abrasive particles are responsible for the jet’s cutting ability, which occurs through erosion. In softer materials, high-pressure water contributes to the cutting action.
The Cutting Head
The orifice, mixing chamber, and mixing tube together constitute what is commonly referred to as the cutting head (see Figure 3). The cutting head’s design is critical. A worn head or inefficient head design can reduce maximum possible cutting speed by between 10 and 20 percent.
A cutting head that consistently shoots a jet from the orifice down the middle of the focusing tube (called alignment) coupled with efficient mixing-chamber design, ensures good cutting performance. The alignment also prevents the focusing tube from prematurely wearing and ensures energy is not wasted by the jet deflecting off the focusing tube’s interior wall.
To balance the head’s performance with operating life, the focusing tube’s inner diameter is usually recommended to be three times the diameter of the jewel orifice. For example, a 0.010-in. orifice would be coupled with a 0.030-in.-inner-diameter mixing tube. (Note: The terms mixing tube and focusing tube are used interchangeably in the waterjet industry.)
Pressure and Velocity
Does higher pressure translate to faster cutting speeds, lower cost per part, and consequently higher productivity? To answer this question, we first need to define some terms, including the available power of the jet. As defined by waterjet manufacturers, power can be represented in the following equation, where K is a constant, P is pressure, and A is the cross-sectional area of the orifice:
Power = K × P15 × A
From the equation it is clear that for a constant power, a higher pressure uses a smaller orifice size, and a larger orifice size will only support a lower pressure. For example, a 50-HP pump running at 60,000 PSI will run a maximum orifice size of 0.014 in. with a greater flow rate; using the same horsepower at 90,000 PSI will run a maximum orifice size of 0.010 in. with a reduced flow rate.
If both jets have the same power, where does the increased cutting speed potential factor in? The answer can be found by simplifying the equation further, dividing power by the cross-sectional area of the jet (A) to give us the power density (Pd). As before, K is a constant and P is pressure.
Pd = K × P15
Power from the earlier equation is dependent on pressure and volume, but power density is dependent only on the pressure the pump is generating and, by extension, the jet velocity.
Recall the physics of an abrasive waterjet operation. The abrasive particles are accelerated by the high-velocity water stream; the higher the jet velocity, the faster the abrasive particles exit the mixing tube, and the greater the power density.
This increased power density of the 90-KSI jet enables faster cutting speeds. Put another way, a higher pressure leads to a higher-velocity water stream, faster abrasive particles, and, ultimately, faster cutting.
Abrasive Usage
Abrasive has significant influence on the operational efficiency of an abrasive waterjet and a major part of the operational cost. Typical applications use garnet as abrasive, which is alluvial (loose, as on beaches) or mined and chemically inert.
Abrasives are measured in mesh sizes, a reference to the processing screen sizes, with larger mesh numbers indicating finer abrasives. For example, 220 mesh has finer particles than 80 mesh. Cutting brittle materials like glass might require softer abrasives like olivine to prevent chipping and cracking, which is why it is important to match the abrasive to the application.
Every mesh number has a range (or distribution) of particle sizes, and care has to be taken in choosing a focusing tube to prevent clogging from oversized abrasive particles. As a general rule, the focusing tube inner diameter should be three times the size of the largest abrasive particle in the distribution.
A waterjet stream at a given pressure has a finite number of abrasive particles that can be added to it before the particles start getting in each other’s way. Too much abrasive reduces the momentum transfer efficiency and slows the cutting speed. This limit is commonly referred to as the peak loading ratio or maximum abrasive feed rate. The larger the orifice size and flow through the orifice, the greater the abrasive feed rate required to reach the maximum cutting power of the jet. This also factors into the overall cost per part. The more abrasive the process uses, the higher the cost per part.
Going back to the 50-HP example with the lower flow rate of the 0.010-in. orifice at 90 KSI, when the jet is at its peak loading ratio, the jet has maximum cutting power. For the same horsepower at 60-KSI pressure, the jet from the 0.014-in. orifice is still not at its peak loading ratio because of the higher flow rate. At 60 KSI, the process requires additional abrasive to reach its peak and, hence, more total abrasive usage, which affects the cost of the operation and the cost per part.
In summary, higher pressure leads to less abrasive required to reach maximum cutting power, which leads to less abrasive use and a lower cost per part.
Kerf Width
An important part of any waterjet cutting conversation is the influence of kerf width. What is kerf width? In simple terms, it is the width of the material that is being removed during the cutting process. The larger the orifice, the wider the kerf.
Especially when cutting expensive material, waterjet cutting a wide kerf really does not have any advantages. The high power density, small orifice, and narrow kerf of a 90-KSI system help control the abrasive waterjet around tight radii and corners (see Figures 4 and 5). Adjustments can be made to lower-KSI waterjet systems with larger orifices, like reducing the ratio of focusing tube diameter to orifice diameter closer to 2.0—that is, a 0.014-in. jet would use a 0.030-in. focusing tube. This can, however, reduce the life of the focusing tube, since more abrasive particles come in contact with the tube walls during the refocusing function.
Deciding the Right Pressure
Higher pressures influence the ability of an abrasive waterjet to cut faster, but this question often is asked: Will higher pressures result in shorter maintenance cycles and decreased component life, increasing cost per part? It would, if you were running a pump designed for 60,000 PSI at 90,000 PSI.
A new generation of 90,000-PSI waterjet pumps are designed to operate at these ultrahigh pressures. The average component lifetimes on current 90-KSI pumps are comparable to component lifetimes on 60-KSI pumps, resulting in similar maintenance cycles, and waterjet pump manufacturers offer maintenance contracts. Though as with many new technologies, some 90-KSI waterjet pumps have limitations on the use of in-house or third-party providers for certain maintenance tasks.
That said, waterjet pump technology continues to march forward, and the pressure is on. The decision rests less on the pressure the pump has to be operating at, 60 KSI or 90 KSI, but more on how to operate the 90-KSI pump in tune with the shop’s productivity requirements.
Images courtesy of KMT Waterjet Systems.
About the Author
Related Companies
subscribe now
The Fabricator is North America's leading magazine for the metal forming and fabricating industry. The magazine delivers the news, technical articles, and case histories that enable fabricators to do their jobs more efficiently. The Fabricator has served the industry since 1970.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 05/14/2024
- Running Time:
- 62:12
Cameron Adams of Laser Precision, a contract metal fabricator in the Chicago area, joins the podcast to talk...
- Trending Articles
A visit to Automate 2024 reveals the future might be now
Why employee-owned companies make sense in manufacturing
What software automation means for custom fabrication
Majestic Steel Arkansas fully operational
Nucor’s weekly steel price announcement continues to rattle markets
- Industry Events
Laser Welding Certificate Course
- May 7 - August 6, 2024
- Farmington Hills, IL
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,