- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Finding the perfect die opening
Use an optimal die opening to make your press brake operation more consistent
- By Steve Benson
- February 15, 2013
- Article
- Bending and Forming
Bottom bending and coining “stamp” the inside bend radius into the part. In air forming, the inside bend radius is “floated” as a percentage of the die opening. Once we determine the radius, we can calculate the required bend deductions.
But how do we find the perfect die opening, one that will establish the radius we want to achieve regardless of the method of forming? You may ask, “Why should I care? If I’m bottoming or coining, I am going to force the punch, material, and die together and stamp the radius. In this case, the die opening will not make much difference in establishing the bend radius. And in an air form, I canjust calculate the inside radius by using the 20 percent rule, establishing the inside radius based on a percentage of the die opening and material type.
“So again, why then should I care?”
To answer that question, let’s first look at what happens when you bend a piece of sheet metal in any of the standard die shapes: V die, acute V die, or channel die, as shown in Figure 1.
The Drawing Process
Have you ever looked at the back side of a bend and noticed the die markings on both sides of the workpiece? These marks are caused by the drawing process—that is, the dragging of material over the top edges of the die and into the die space. This is not the same type of drawing found in hydroforming or deep-draw stamping; no real stretching of the material is occurring.
Besides the die marking, something else may be occurring in some materials. The bending process could be creating a secondary radius that is unique from the radius that you are trying to attain. This secondary radius has a direct relationship to the die opening. The larger the die opening is in relationship to the material thickness, the greater this secondary radius can become (seeFigure 2).
You will not see this radius once the bend is completed. But this secondary radius can and sometimes does manifest itself as bend angle, making the bend appear to have a greater angle than is actually being produced in the sheet metal itself. This effect can work for you or against you, depending on how it is applied. Knowing that this extra radius is possible and how to work with it can makeor break a part.
This effect can be a particularly big issue if you are bottom bending. If you are bottoming in a large die opening and this extra radius is occurring, it can manifest itself as extra bend angle, and this may create a problem. In bottoming, the bend is brought up to the desired bend angle plus a degree or two for springback, just like in air forming. But rather than releasing the material as inan air form, bottom bending continues down with the tool into the die space until the desired depth is achieved, forcing the overbent material back to the die angle, which in bottoming is usually 90 degrees. This effect is known as spring forward, as opposed to springback.
Because the bottoming process overbends and then forces the material back to the set angle of the die, when the estimated depth of penetration is reached, the part is removed and checked, and we find that the bend is still overbent. And because we first overbent the part and are now forcing the material back open, we may think we need to hit the part harder to force the material to the setangle.
But the overbend may never be forced out, no matter how much pressure is applied. This is because it has nothing to do with what is occurring at the bottom of the bend. If the technician does not realize that this may be happening, he or she could eventually overtonnage the press brake and/or the tooling while never achieving the desired results.
There is a big difference between an optimal die opening that is geometrically perfect and the actual die you are going to use. Still, we want to get as close as possible to perfect, for numerous reasons—like the one just described. To find the best working die opening, without just guessing, you will need a starting point.
You will find that best starting point by making a couple of minor assumptions about the bend. The first is that the bend has 90 degrees of bend angle, regardless of what the bend angle really is. This will give a good starting number and simplify the calculations, allowing you to work with a 45-degree right triangle.
The Perfect Die Opening
When it comes to any kind of machine, you generally do not want to overuse or underuse it. You get the most value at half of the maximum working value. That being said, isn’t the combination of die, punch, and material really a “machine”? Of course it is. So, let’s look at the die and try to determine how we use it to half its working value.
So what is half the working value of a die? Under perfect conditions, that point occurs halfway down the die face, as shown in Figure 3. This is the point where we want the material to separate from one side of the die, at the tangent point on the bend, and rejoin the die on the opposite face.
In a perfect die opening, this halfway point down the die face is exactly twice the bend’s outside setback (OSSB). The OSSB is the distance from the tangent of the radius and the leg (flat) to the apex of the bend. In this situation, we find that we have an OSSB from the tangent point down to the bend apex, and an OSSB from that tangent point up to the top of the die. You are holding the partgeometrically perfect in the die opening.
This makes finding the optimal die opening easy. Again, we’re assuming that the bend angle is 90 degrees, whether it is or isn’t. This means we’re working with a right-angle triangle. When working with a 90-degree bend, the OSSB also is equivalent to the outside bend radius. So if you know the outside bend radius, there’s no need to calculate the OSSB. Double the outside bend radius, and youhave the hypotenuse of a 45-degree right triangle. From there it is a simple process to determine the die opening, as shown in Figure 4.
All this can be simplified to the following equation: Geometrically perfect die opening = (Outside radius × 0.7071) × 4. If we apply this to the example in Figure 4, we get: (0.150 × 0.7071) × 4 = 0.424 in. To deal with springback, we increase the multiplier a little (and, hence, the die opening). In material thicknesses less than 0.125 in., a realistic working multiplier is 4.85, as in:(Outside radius × 0.7071) × 4.85. In material between 0.125 and 0.250 in., the multiplier is 5.85 in., because of tonnage requirements and the possibility of increasing springback of thicker materials. (Material more than 0.250 in. thick is calculated differently.)
Editor's Update: Since this article was published, Benson has proposed another formula for determining the optimum die width: Outside bend radius × 3.29435. For more on this, click here.
There Is No Perfect Die, So Now What?
It is rare that an optimal die width is actually available. For instance, if you find that the perfect die opening is 0.424 in., the closest available die may be either one with a die opening of 0.395 in. or one with an opening of 0.472 in.
For the final selection, the closer we can get to perfect the better, but this may not always be practical. In this example, 0.395 in. is closest, but it may be too small from a tonnage perspective, depending on the forming method, material type, material thickness, and length of bend. You always need to check and make sure that you do not overtonnage your machine or your tooling. If thetonnage is acceptable, you can use the closest die opening. If it’s not acceptable, you must use a larger die opening.
This die selection method is valid for all three methods of forming—coining, bottoming, and air forming—and will, for the most part, keep the relationships between the die width and outside bend radius whether the material is thick with a small radius, thin with a large radius, or there is a 1-to-1 relationship between material thickness and the radius.
In the past, the rule of thumb has been that eight times the material thickness is a perfect die opening—which it is, but only in a 1-to-1 relationship between the inside bend radius and the material thickness: for instance, an 0.062-in. radius in 0.062-in.-thick material. But what if the material is 0.036 in. with a 3-in. radius? Will eight times the material work? No, eight times thematerial thickness will not produce a valid or acceptable die opening for a radius this large.
Benefits of a Perfect Die Opening
There are several other reasons for finding the perfect die opening. First, it keeps the material and inside radius relationships the same, and so the technician will be able to make adjustments to the controller in a more consistent manner over time.
For example, if you are working with a die opening that’s as close to perfect as possible, you may find it consistently takes, hypothetically speaking, 0.005 in. to achieve 1 degree of angular change. Using a larger-than-necessary die, it may take 0.020 in. to achieve the same angular change. This means that the punch will need to go farther down into the V to achieve a degree of angularchange (see Figure 5).
An optimal working die opening also helps when you use shims or an angular compensation device to create an angular change. Using an optimal working die opening will require only a small amount of movement to bring about a degree of angular change, and you’ll need only light crowning.
But if it takes more movement to create angular change (for example, 0.020 in.), then you will need more shimming. If you need to shim the larger die or use an angle compensation device, it may not work so well. You may exceed the ability of the compensation device or, worse yet, create the need to place so many shims under the die that you end up putting a reverse crown into the die itself(see Figure 6).
On the other hand, you may want to use a larger die opening from time to time just to stabilize a specific forming project. For instance, you may want to account for variations in material properties. If the material thickness varies ±0.010 in. and it takes 0.020 in. of ram movement to cause a degree of angular change, then the angular error will be only 0.5 degree. However, the techniciancannot make the decision to use a larger die on his own; the part would need to be designed for the larger radius produced by air forming in a larger opening.
There are many more examples of why using a die opening as close to perfect as possible is worth the time and effort. Nonetheless, by staying as close as possible to perfect, your forming consistency will improve, your setup and run-times will get shorter, and the risks of running into problems will be greatly reduced.
About the Author
Steve Benson
2952 Doaks Ferry Road N.W.
Salem, OR 97301-4468
503-399-7514
Related Companies
subscribe now
The Fabricator is North America's leading magazine for the metal forming and fabricating industry. The magazine delivers the news, technical articles, and case histories that enable fabricators to do their jobs more efficiently. The Fabricator has served the industry since 1970.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 05/14/2024
- Running Time:
- 62:12
Cameron Adams of Laser Precision, a contract metal fabricator in the Chicago area, joins the podcast to talk...
- Trending Articles
Press brakes, panel benders, and flat blank calculations
Nucor’s weekly steel price announcement continues to rattle markets
Educating, rather than just training, tomorrow's workforce
Washington artist creates life-size elk sculptures
Universal Robots, MiR open robotics hub in Denmark
- Industry Events
Laser Welding Certificate Course
- May 7 - August 6, 2024
- Farmington Hills, IL
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,